Precipitaion Ho thatafatsa tšepe e sa hloekang
Alloy e phahameng ea mocheso
◆0Cr17Ni7Al ke tšepe e thatafatsang pula e nang le Al e kenyellelitsoeng, e sebelisoang e le liliba, li-washer, likarolo tsa calculator, joalo-joalo.
◆0Cr15Ni7Mo2Al e sebelisetsoa lijana tse matla haholo, likarolo le likarolo tsa sebopeho tse nang le litlhoko tse itseng tsa ho hanyetsa kutu.
◆ Ts'ebetso ea 0Cr15Ni5Cu4Nb e tšoana le ea 0Cr17Ni4Cu4Nb, empa e na le ts'ebetso e ntle ea lateral.
◆0Cr12Mn5Ni4Mo3Al (Gangyan 69111) e na le polasetiki e ntle ho feta 0Cr15Ni7Mo2Al.
◆0Cr17Ni4Cu4Nb Precipitation e thatafatsa tšepe e nang le Cu e ekelitsoeng, e sebelisoang haholo ka li-shafts, likarolo tse phahameng tsa sebopeho tse hlokang ho hanyetsa ho bola bakeng sa likarolo tsa turbine tsa mouoane.
◆XM-25 e hanela mocheso le mocheso o phahameng, e loketse petroleum, lik'hemik'hale, sepakapaka, matla a nyutlelie le liindasteri tse ling.
Sebopeho sa lik'hemik'hale
Kereiti | C | Si | Mn | S | P | Cr | Ni | Mo | Cu | Nb | Al | tse ding |
ha e kholo ho feta | ||||||||||||
0Cr17Ni4Cu4Nb | 0.07 | 1 | 1 | 0.035 | 0.03 | 15.5 ho isa ho 17.5 | 3 - 5 | - | 3 - 5 | 0.15–0.45 | - | - |
0Cr17Ni7Al | 0.09 | 1 | 1 | 0.035 | 0.03 | 16-18 | 6.5 ho isa ho 7.5 | - | ≤0.5 | - | 0.75-1.5 | - |
0Cr15Ni7Mo2Al | 0.09 | 1 | 1 | 0.035 | 0.03 | 14-16 | 6.5 ho isa ho 7.75 | 2 - 3 | - | - | 0.75-1.5 | - |
0Cr15Ni5Cu4Nb | 0.07 | 1 | 1 | 0.035 | 0.03 | 14 ho isa ho 15.5 | 3.5 ho isa ho 5.5 | - | 2.5 ho isa ho 4.5 | 5*C%~0.45 | - | - |
0Cr12Mn5Ni4Mo3Al | 0.09 | 0.8 | 4.4 ho isa ho 5.3 | 0.03 | 0.03 | 11-12 | 4 - 5 | 2.7 ho isa ho 3.3 | - | - | 0.5 ~ 1 | - |
XM-25 | 0.05 | 1 | 1 | 0.03 | 0.03 | 14-16 | 5 - 7 | 0.5 ~ 1 | 1.25 ho isa ho 1,75 | ≥8*C% | - | - |
Bonyane ba thepa ea alloy
Kereiti | naha | matla a tsitsitseng RmN/m㎡ | Yield Strength Rp0.2N/m㎡ | Elongation As% | HRC(HBS) |
0Cr17Ni7Al | tharollo e tiileng 1000~1100℃ho pholisa ka potlako | ≤1030 | ≤380 | ≥20 | ≤229 |
565℃botsofali | ≥1140 | ≥960 | ≥5 | ≥363 | |
510℃botsofali | ≥1230 | ≥1030 | ≥4 | ≥388 | |
0Cr17Ni4Cu4Nb | 480℃ ho tsofala | ≥1310 | ≥1180 | ≥10 | ≥40 |
550℃botsofali | ≥1060 | ≥1000 | ≥12 | ≥35 | |
580℃botsofali | ≥1000 | ≥865 | ≥13 | ≥31 | |
620℃botsofali | ≥930 | ≥325 | ≥16 | ≥28 | |
0Cr15Ni5Cu4Nb | tharollo e tiileng | - | - | - | ≤380 |
565℃botsofali | ≥1210 | ≥1100 | ≥7 | ≥375 | |
510℃botsofali | ≥1320 | ≥1210 | ≥6 | ≥388 | |
0Cr12Mn5Ni4Mo3Al | 520℃botsofali | ≥1520 | ≥1280 | ≥9 | ≥47 |
XM-25 | 560℃botsofali | ≥1100 | ≥1000 | ≥10 | ≥45 |